BF17 and BF05 share the same 98–99% hydrolysis - chemically they are siblings. The single difference is chain length, and it changes almost everything downstream: how much solids you can run, how deep the solution penetrates, how strong the dried film is, and ultimately which applications each grade can serve.
This comparison walks through both grades side by side, explains what viscosity actually does in a process, and ends with an application-by-application mapping so you can pick the right grade - or decide to blend.
1. The two grades at a glance
| BF17 | BF05 | |
|---|---|---|
| Also known as | PVA 1799, 28-98, Wanwei 100-27, Kuraray PVA-117, Mowiol 30-98, Selvol 325 | PVA 0599, 5-98, Sundy 098-05, Kuraray PVA-105, Mowiol 4-98, Selvol 305 |
| Degree of polymerization | ≈ 1,700 | ≈ 500 |
| Degree of hydrolysis | 98.5–99.2 mole% | 98.5–99.2 mole% |
| Viscosity (4% aq., 20 °C) | 25–30 mPa·s | 5–6 mPa·s |
| Dissolution | 80–95 °C, slower (60–90 min hold) | 80–95 °C, faster (30–60 min hold) |
| Film strength | High | Moderate |
| Penetration into porous surfaces | Lower | High |
| Main applications | Warp sizing, adhesives, paper, electrode binders | Paper surface sizing, pigment coating, PVA sponge, mold release, abrasives |
Both are fully hydrolyzed: hot-water soluble, water-resistant when dry, and the strongest film formers in the PVA family. Neither will dissolve in cold water. The question is never hydrolysis - it is viscosity.
2. What viscosity actually changes
Solution viscosity rises steeply with both polymer chain length and solids content. That one relationship drives four practical consequences:
- Working solids. A 15% solution of BF17 is already thick and hard to pump; a 15% solution of BF05 still flows like thin syrup. If your process needs a high-solids liquor - fast build on the substrate, less water to evaporate - BF05 makes it possible.
- Penetration. Thin solutions wick into porous surfaces (paper, unglazed ceramics, fiber) before they gel. BF05 penetrates deeply, which is why it anchors pigment on paper and bonds grit to sandpaper backing. BF17 sits more on the surface, building a stronger film there instead.
- Film strength per pass. Longer chains make tougher, more extensible films. BF17 films resist abrasion better - the property that makes it the warp-sizing workhorse. BF05 films are weaker alone but can be built up in multiple passes or blended up.
- Dissolution speed. Short chains hydrate and untangle faster. BF05 cooks in roughly half the time of BF17 at the same temperature - a real saving in plants that cook several batches per shift.
3. Which grade for which job
| Application | Recommended | Why | Typical dosage |
|---|---|---|---|
| Cotton / poly-cotton warp sizing | BF17 | Abrasion-resistant film protects yarn through weaving | 20–60% of size solids |
| Fine filament sizing | BF17 (or blend with 2699) | Higher DP for maximum film strength | 20–60% of size solids |
| Paper surface sizing | BF05 | 4–8% liquor at the size press without throwing | 4–8% solution |
| Pigment coating binder | BF05 | Deep penetration, high gloss at low addition | 2–5 phr |
| PVA sponge | BF05 | Fine, uniform cell structure from low viscosity | 8–12% solution |
| Wood / paper solution adhesives | BF17 | Strong bond and film from medium-DP chains | 10–20% solids |
| PVAc protective colloid | Blend (BF05 + BP grades) | Fine particle size plus emulsion stability | 4–8% on monomer |
| Mold release for FRP | BF05 | Thin solution, slick water-soluble parting film | 5–10% solution |
| Electrode binder | BF17 | Tougher film holds active material together | per formulation |
| Abrasives / sandpaper star coat | BF05 | Penetrates backing before gelling | 10–15% solution |
Full grade details: PVA BF17 guide and PVA BF05 guide.
4. Can one substitute for the other?
Sometimes, and the direction matters:
- BF05 instead of BF17 works where the process has heating, film strength demand is moderate, and penetration is welcome - e.g. switching a paper sizing recipe. It usually fails where abrasion resistance is the point: a warp-sizing size box filled with BF05 will shed film into the creel and under-protect the yarn.
- BF17 instead of BF05 fails for the opposite reason: at the solids your BF05 recipe runs, BF17 solution is too thick to pump, and the film sits on the surface instead of penetrating. You can run BF17 at lower solids, but then you pay in drying load.
- Blending is the normal answer when one grade alone is not quite right - e.g. a 70/30 BF17/BF05 blend for sizing yarns that need surface build without brittleness. Blends of fully and partially hydrolyzed grades (BF17 + BP17) are also common where a little cold-water sensitivity is acceptable in exchange for easier cooking.
5. The commercial angle
Both grades are commodity chemicals with active competition between Chinese producers, so the lever is not availability - it is specification discipline. Two checks keep a grade switch honest:
- Verify hydrolysis and viscosity on the COA of the actual batch, not the brochure. The 4%-solution viscosity range is the property most likely to drift between producers.
- Run a plant trial before switching containers. Lab cooks hide the differences that matter - pump behaviour, foam, first-pass film quality. A one-pallet trial (800–1,000 kg) is cheap insurance.
For dissolution procedures and hold times for both grades, see how to dissolve fully hydrolyzed PVA. Product pages with full TDS: PVA BF17 and PVA BF05.
6. Quick decision checklist
- Does the film need to survive abrasion (yarn through heddles)? → BF17
- Do you need maximum solids in the liquor to cut drying cost? → BF05
- Is the substrate porous and the bond dependent on penetration (paper, grit, sponge)? → BF05
- Is the solution's job to sit on the surface and build a coating (warp sizing, electrode film)? → BF17
- Cook time per shift a bottleneck? → BF05 (or accept longer holds with BF17)
- Not sure? → describe the line to our technical team; a grade recommendation with sample support takes a day.
Frequently asked questions
What is the main difference between PVA BF17 and BF05?
Chain length. BF17 has a degree of polymerization around 1,700 (viscosity 25–30 mPa·s at 4%); BF05 around 500 (5–6 mPa·s). Hydrolysis is identical at 98–99%. Everything else - working solids, penetration, film strength, dissolution speed - follows from that difference.
Is BF05 just diluted BF17?
No. Dilution lowers concentration, not chain length. A 4% BF17 solution and an 8% BF05 solution may have similar viscosity, but the films they form and the way they penetrate substrates are completely different. Grades cannot be replicated by dilution.
Which grade is cheaper per ton?
Prices of the two grades track each other closely; BF05 sometimes carries a small premium because its production volume is smaller. Total cost, however, is usually decided by the formulation - a grade that runs at higher solids or cuts cook time can be cheaper in use even at a higher unit price.
Can I blend BF17 and BF05?
Yes, and it is common practice. Cook each grade separately (they need different hold times) and combine hot, or add BF05 to a hot BF17 cook 20 minutes before discharge. Blends tune film strength and penetration between the two endpoints.
Do both grades need hot water?
Yes. Both are 98–99% hydrolyzed and require 80–95 °C to dissolve fully; neither works in cold-water processes. For cold-soluble requirements, use partially hydrolyzed grades such as BP17 or BP24 - see the partially hydrolyzed PVA range.